DIN EN ISO 6931-1 – stainless steel spring wires, steel grades, properties and tolerances
DIN EN ISO 6931-1:2020-11 specifies the technical requirements for stainless steel spring wires with a round cross-section intended for the production of springs, spring elements and mechanical parts exposed to corrosion. The standard covers primarily cold-drawn wires, for which tensile strength, surface quality, dimensional accuracy and repeatability of mechanical parameters are important.
DIN EN ISO 6931-1:2020-11 is the German implementation of EN ISO 6931-1:2020, which is based on the international standard ISO 6931-1:2016. It replaces the previous standard DIN EN 10270-3.
Scope of the DIN EN ISO 6931-1 standard
This standard applies to corrosion-resistant steel wires used in technical springs and components operating under elastic loads. It specifies requirements for:
- round wires with a nominal diameter of up to 10 mm,
- possibility of ordering diameters above 10 mm up to 15 mm after agreeing on mechanical properties,
- chemical composition of individual species,
- tensile strength and strengthening level,
- tolerances on diameter, ovality and length of cut sections,
- surface quality and acceptable methods of finishing,
- delivery conditions, tests and acceptance documents.
The material range includes primarily austenitic steels, as well as selected duplex and precipitation-hardened steels. The general technical delivery conditions are supplemented by the ISO 404 standard.
Steel grades according to DIN EN ISO 6931-1
The standard lists eight grades of stainless steel, divided according to their structure and the way they obtain their elastic properties. The table shows their material designations and the ISO designations used in the document.
| Stainless steel grades – ISO 6931-1 | |||
| EN grade | ISO designation | Structure | Characteristic |
| 1.4310 X10CrNi18-8 | 4310-301-00-I | Austenitic | High cold-drawn strength |
| 1.4325 X9CrNi18-9 | 4325-302-00-E | Austenitic | Chrome-nickel steel for spring wires |
| 1.4315 X5CrNiN19-9 | 4315-304-51-I | Austenitic | Alloy steel with added nitrogen |
| 1.4301 X5CrNi18-10 | 4301-304-00-I | Austenitic | Universal Cr-Ni steel |
| 1.4401 X5CrNiMo17-12-2 | 4401-316-00-I | Austenitic | Increased corrosion resistance thanks to Mo |
| 1.4539 X1NiCrMoCu25-20-5 | 4539-089-04-I | Austenitic | High-alloy Ni-Cr-Mo-Cu steel |
| 1.4462 X2CrNiMoN22-5-3 | 4462-318-03-I | Duplex | High strength and corrosion resistance |
| 1.4568 X7CrNiAl17-7 | 4568-177-00-I | Precipitation hardened | 17-7PH, can be hardened by heat treatment |
1.4310 – X10CrNi18-8 is one of the most commonly used grades for the production of stainless steel spring wires. Cold-work hardening during cold drawing gives it high tensile strength and good performance in mechanical springs.
1.4301 – X5CrNi18-10 It is an alternative in applications requiring corrosion resistance and appropriately selected mechanical parameters. However, it should not be assumed that 1.4301 wire automatically has the same elastic characteristics as 1.4310.
1.4401 – X5CrNiMo17-12-2 contains molybdenum, which improves resistance to pitting corrosion, especially compared to classic chromium-nickel steels. In practice, the grade 1.4404/316L, however, it should not be automatically identified with the grade 1.4401 mentioned in the standard.
1.4462 – X2CrNiMoN22-5-3 is an austenitic-ferritic duplex steel characterized by high mechanical strength and good corrosion resistance. Its use requires consideration of technological properties and forming conditions.
1.4568 – X7CrNiAl17-7, also known as 17-7PH, is a precipitation-hardening steel. The final properties of the spring depend not only on the condition of the wire after drawing, but also on the heat treatment applied.
17-4PH and martensitic steels and the ISO 6931-1 standard
Other stainless steels, the properties of which are obtained by hardening or precipitation hardening, can also be used in the production of spring elements.
An example is 1.4542 / 17-4PH, as well as martensitic steels such as 1.4122 in 1.4005.
However, these are not the grades listed in the basic material table ISO 6931-1:2016. Their use in the production of springs requires a separate definition of mechanical properties, delivery condition and technical requirements.
Mechanical properties of stainless steel spring wires
The basic mechanical parameter defined by the standard is tensile strength Rm, expressed in MPa. Its required value depends on the steel grade, wire diameter and strength level.
Two levels are provided for selected species:
- NS (Normal Strength) – normal level of tensile strength,
- HS (High Strength) – increased level of tensile strength.
These designations should not be confused with separate steel grades. They define the mechanical requirements for the material in its respective delivery condition.
Tensile strength Rm – 1.4310 steel
The table below shows selected tensile strength ranges for 1.4310 stainless steel wire in the cold drawn condition, for NS and HS levels according to ISO 6931-1.
| Strength Rm – steel 1.4310 [MPa] | ||
| Diameter d (mm) | NS | HS |
| d ≤ 0,20 | 2200–2530 | 2350–2710 |
| 0,40 < d ≤ 0,50 | 2050–2360 | 2200–2530 |
| 0,80 < d ≤ 1,00 | 1900–2190 | 2050–2360 |
| 1,75 < d ≤ 2,00 | 1700–1960 | 1850–2130 |
| 3,50 < d ≤ 4,25 | 1500–1730 | 1600–1840 |
| Warning: The table contains selected diameter ranges and is used to compare NS and HS levels. Full requirements, including other diameters, testing principles, and permissible deviations within a production batch, are specified in ISO 6931-1. Higher tensile strength does not automatically mean greater fatigue life for the finished spring. Geometry, surface quality, operating stresses, corrosive environment, and manufacturing process also influence its performance. | ||
Wire diameter tolerances according to DIN EN ISO 6931-1
Dimensional accuracy requirements depend on the nominal wire diameter and tolerance class. The standard specifies classes T12, T13, T14, and T15 for wires supplied in coils or on spools.
A lower tolerance indicates greater diameter accuracy. Grade T15 is more stringent than grade T14 and should be clearly specified in the order if required.
| Tolerances of wire diameter in coils and on spools [mm] | ||
| Nominal diameter d | Class T14 | Class T15 |
| d ≤ 0,20 | ±0,005 | ±0,004 |
| 0,25 < d ≤ 0,40 | ±0,008 | ±0,005 |
| 0,64 < d ≤ 0,80 | ±0,010 | ±0,008 |
| 1,00 < d ≤ 1,60 | ±0,015 | ±0,010 |
| 2,25 < d ≤ 3,19 | ±0,020 | ±0,015 |
| 4,50 < d ≤ 6,00 | ±0,025 | ±0,020 |
| 9,00 < d ≤ 10,00 | ±0,035 | ±0,030 |
| The values provided apply to selected dimensional ranges. Other ranges and classes T12 and T13 are specified in the relevant standard table. Separate diameter and length tolerance rules apply to straightened and cut wires. In applications requiring high precision, not only the diameter tolerance but also the requirements for ovality and straightness must be agreed. | ||
Surface condition of spring wires
Surface condition has a significant impact on the fatigue life and corrosion resistance of spring wires. Cracks, fractures, inclusions, and other discontinuities can act as stress concentration points, especially during cyclic loading.
Depending on the arrangements between the manufacturer and the customer, wires can be supplied with different surface finishes, e.g. uncoated, polished or with a specific technological coating.
The standard does not automatically mean that all wires must be supplied in a passivated condition. The required surface condition should be clearly specified when submitting an inquiry or order.
Testing and quality control according to ISO 6931-1
Spring wire inspections include mechanical properties, chemical composition, dimensions, and technological characteristics. The scope of testing depends on the requirements of the standard and the order documentation.
| Testing of stainless steel spring wires | |
| Type of study | Purpose and requirements |
| Tensile test | Determination of Rm; ISO 6892-1 method |
| Chemical composition analysis | Confirmation of species-specific composition; sampling according to ISO 14284 |
| Dimensional control | Diameter, ovality, tolerances and section lengths |
| Technological research | Winding, wrapping or bending test in accordance with the requirements of the standard |
| Surface assessment | Inspection for defects and required surface finish |
| Acceptance documentation | Control documents according to ISO 10474, e.g. certificate 3.1 |
Requirements for technological testing are particularly important in the case of wires intended for forming springs with small bending radii or complex geometry.
Spring wire delivery terms
Information necessary for ordering
When ordering stainless steel wires according to ISO 6931-1, the following must be clearly stated:
- quantity of material ordered,
- steel grade and standard designation,
- NS or HS strength level, if applicable to a given species,
- nominal diameter and tolerance class,
- the form of delivery and the possible length of the sections,
- required surface condition and type of coating,
- type of acceptance document, e.g. 3.1,
- agreed additional technical requirements.
Example of the marking of the ordered wire:
Spring wire 1.4310 / ISO 6931-1 / 4310-301-00-I / NS / Ø2,50 mm / T15 / coil / certificate 3.1.
A correctly formulated order reduces the risk of delivering material with an incorrect level of strengthening, dimensional tolerance or surface condition.
Form and method of delivery
Stainless steel spring wires can be supplied, among others, as:
- vertebrae and coils,
- wires on spools,
- wires on transport carriers,
- sections straightened and cut to size.
For coil deliveries, the winding parameters are also important, including the geometry and behavior of the wire after unwinding. For straightened sections, the requirements regarding straightness and length are particularly important.
Functional properties and selection of steel grades
Austenitic steels
Austenitic steels, such as 1.4310, 1.4301, and 1.4401, are widely used in the production of corrosion-resistant springs. Their mechanical properties can be adjusted through cold drawing and appropriate technological processes.
The typical modulus of elasticity (E) for these steels is around 190–200 GPa, but the specific design value should be selected based on the grade and operating conditions. The modulus of elasticity is not the same as tensile strength.
Duplex steel
Duplex steels, such as 1.4462, combine austenitic and ferritic structures. They are characterized by high strength and good resistance to certain forms of corrosion, including stress corrosion cracking in certain chloride environments.
When designing springs from these materials, their formability and technological requirements must be taken into account.
Precipitation hardening steels
The 1.4568 / 17-7PH grade enables high mechanical parameters to be achieved thanks to the appropriate combination of cold deformation and heat treatment.
The parameters of the finished spring should be assessed based on the actual state of the material after the manufacturing process. The properties of the wire itself before heat treatment do not fully determine the properties of the finished part.
Applications of stainless steel wires according to DIN EN ISO 6931-1
Stainless steel spring wires are used to produce components operating under constant or variable loads, also in environments requiring increased corrosion resistance.
Typical applications include:
- compression, extension and torsion springs,
- precision springs for mechanisms and devices,
- spring rings and securing elements,
- clips, pins, snaps and clamping elements,
- elements of industrial and measuring equipment,
- components for the food and chemical industries,
- selected elements of medical devices,
- parts of mechanisms operating in humid environments.
The grade selection should take into account mechanical requirements, the presence of corrosive factors, operating temperature and the expected number of load cycles.
The importance of DIN EN ISO 6931-1 in industrial practice
Applying uniform technical requirements enables comparisons of spring wires from different manufacturers. This is particularly important where springs must maintain consistent mechanical and dimensional properties.
The DIN EN ISO 6931-1 standard establishes a common reference point for the manufacturer, supplier, and recipient of the material. It reduces the risk of errors resulting from ambiguous specifications of the grade, tolerance class, or strength level.
However, it should be remembered that compliance of the wire itself with the standard does not replace fatigue life analysis, operating conditions or testing of the finished spring.
Stainless steel spring wires – Alfa-Tech
When selecting stainless steel spring wire, the material type, diameter, required tensile strength, dimensional accuracy and operating conditions are of particular importance.
Also check out information about stainless steel spring wires 1.4310 and 1.4301, their material designations, properties and applications.
Related standards and technical sources
- ISO 6931-1:2016 – Stainless steels for springs – Part 1: Wire.
- EN ISO 6931-1:2020 – European implementation of the standard.
- DIN EN ISO 6931-1:2020-11 – German edition of the standard.
- ISO 404 – general technical conditions of delivery of steel products.
- ISO 6892-1 – tensile test of metallic materials.
- ISO 10474 – steel product control documents.
- ISO 22034-2 – dimensional tolerances of steel wires.