Po'lat 1.4876, X10NiCrAlTi32-21, Qotishma 800, 800H, 1.4958, 1.4959, 1.4558, X10NiCrAlTi32-20, X5NiCrAlTi31-20, X8NiCrAlTi32-21

1.4876 yuqori qotishmali po'lat – titan va alyuminiy qo'shilgan ostenitik nikel-xromli issiqlikka chidamli po'lat X10NiCrAlTi32-21 PN EN 10095 X5NiCrAlTi31-20, 1.4958, PN EN 10088-1:2007 X8NiCrAlTi32-21, 1.4959, X2NiCrAlTi32-20, 1.4558, X10NiCrAlTi32-20, Incoloy 800, Incoloy 800HT, Alloy 800, Alloy 800H

Materiallar Alfa-Tech 1.4876 / X10NiCrAlTi32-21 / Alloy 800 da mavjud

1.4876 / X10NiCrAlTi32-21 / Qotishma 800 tayoqchalar – issiq prokatlangan, tozalangan va tortilgan
Yassi novlar 1.4876 / X10NiCrAlTi32-21 / Qotishma 800
Soxta armaturalar 1.4876 / X10NiCrAlTi32-21 / Qotishma 800
1.4876 / X10NiCrAlTi32-21 / Qotishma 800 zarblari – ochiq qolipli, zarb qilingan kublar va vallar
Quvurlar 1.4876 / X10NiCrAlTi32-21 / Qotishma 800 – prokatlangan, chok bilan tortilgan, choksiz
1.4876 / X10NiCrAlTi32-21 / Qotishma 800 chiziqlari
1.4876 / X10NiCrAlTi32-21 / Qotishma 800 varaqlari – issiq prokatlangan, sovuq prokatlangan
Simlar 1.4876 / X10NiCrAlTi32-21 / Qotishma 800

telefon: + 48 63 2610519
kontakt@alfa-tech.com.pl

1.4876, X10NiCrAlTi32-21 po'latlarining kimyoviy tarkibini X5NiCrAlTi31-20, 1.4958, X8NiCrAlTi32-21, 1.4959, X2NiCrAlTi32-20, 1.4558, X10NiCrAlTi32-20, Incoloy 800, Alloy 800, Alloy 800H ekvivalentlari bilan taqqoslash. Incoloy 800H, Incoloy 800HT.

Turlar
bo'ldi
 
Norma
Kimyoviy tarkibi (%)
C
Mn
Si
P
S
Cu
Cr
Ni
tug'ma
X10NiCrAlTi32-21 1.4876
PN EN SEW470
max
0,12
max
2,00
max
1,00
max
0,030
 
 
max
0,015
 
 
-
19,00
23,00
30,00
34,00
Ti 0,15-0,60 Al 0.15-0,60 Fe - dam olish
X5NiCrAlTi31-20 1.4958
 
X8NiCrAlTi32-21 1.4959
 
X2NiCrAlTi32-20 1.4558
PN EN
DIN EN
0,03  0,08

0,05 0,10


max 0,03
max
1,50
max
0,70
 
 
max
0,015

max 0,020
 
 
max
0,010

max 0,015
 
 
max
0,50

-
 
 
19,00
22,00

20,00 23,00
30,00 32,50

30,00 34,00


32,00 35,00
Nb max 0,10 Ti 0,20-0,50
Al 0,20-0,50 Co max 0,50 N maksimal 0,03

Ti 0,25-0,65 Al 0,25-0,65
Maksimal 0,50 nima N maksimal 0,03

Al 0,15-0,45 Ti 8 x  (C+N) – 0,60
N08800 UNS N08800
Incoloy® Qotishma 800 (SMC)

ASTM A 240 (800)
ASTM B 366 (N 08800)

N08810 UNS N08810
Incoloy® Qotishma 800H (SMC)

ASTM A 240 (Kechki 800 da)
ASTM A 480 (N 08810)

N08811 UNS N08811
Incoloy® Qotishma 800HT (SMC)

ASTM A 240 (N 08811)
ASTM A 480 (N 08811)
UNS
ASTM
SMC
max
0,10


 

0,50
0,10
 

 
0,60
0,10
max
1,50
max
1,00
max
0,045
max
0,015
max
0,75
19,00
23,00
30,00
35,00
 
 
 
 
Ti 0,15-0,60
Al 0.15-0,60
Fe – minimal 39,5
Al + Ti: 0.30-1.20
 

 
Ti 0,25-0,60
Al 0.25-0,60
Fe – min 39,5
Al + Ti: 0.85-1.20
Nikrofer® 3220 H  Qotishma 800H

Nicrofer ® 3220 H Qotishma 800 ot kuchi

TK
0,06- 0,08

0,06 – 0,10

0,50
1,00
0,20
0,60
max
0,015
max
0,010
max
0,50
19,00-21,00

19,00-22,00

30,00
32,00
Al 0,20-0,40 Ti 0,20-0,50
Al+Ti maksimal 0,70 Fe – qolganlari

Al 0,30-0,60 Ti 0,30-0,60 Al+Ti 0,85- 1,20 Fe- rest

ХН32Т
   HN23T ChN32T KHN32T X20N32T H20N32T Ch20N32T KH20N32T ЭП670 EP670
GOST
max
0,05
max
0,70
max
0,70
max
0,030
max
0,020
max
1,00
18,00
20,00
30,00
34,00
Ti 0,25-0,60 Maksimal 0,50 Issiqlikka chidamli po'latlar guruhidan po'lat
(jaroprochnyy)
NS111
0Cr20Ni32Ti H01110
GB / T
max
0,10
max
1,50
max
1,00
max
0,030
max
0,015
max
0,75
19,00
23,00
30,00
35,00
Ti 0,15-0,60
Al 0.15-0,60
Fe – qolganlari
Z8NC33-21
URANUS® 800H


Z 10 NC 32-21 PHY HT800

AFNOR
0,05 - 0,10

maksimal 0,10

max
2,00
max
0,75
max
0,035
max
0,015
-
19,00
23,00
30,00
35,00
Ti 0,15-0,60
Al 0.15-0,60
Fe – qolganlari

Issiqlikka chidamli po'lat navi 1.4876, X10NiCrAlTi32-21, X5NiCrAlTi31-20 (1.4958), X8NiCrAlTi32-21 (1.4959), X2NiCrAlTi32-20 (1.4558)

Yuqori haroratlarda oksidlanishga chidamliligi yuqori va qattiqligi yuqori bo'lgan ostenitik po'latdir, sanoat pechlarini qurishda, issiqlik bilan ishlov berish qurilmalarida, bug 'qozonlarini qurishda, kimyo sanoatida, neftni qayta ishlashda, issiqlik almashtirgichlar uchun ishlatiladi, havoda maksimal ish harorati 1100 o C.

Issiqlik bilan ishlov berish shartlari X10NiCrAlTi32-21, X5NiCrAlTi31-20, 1.4958, X8NiCrAlTi32-21, 1.4959, X2NiCrAlTi32-20, 1.4558, Qotishma 800H, 800HT

Eritmani 1050 – 1150 o C da tavlash, suv va havo bilan sovutish

O'rtacha sirpanish chegarasi (1000 soat va 10 000 soatdan keyin 1% uzayish)

  • 600 ° C — R1/1000: 130 N/mm² (MPa); R1/10000: 90 N/mm² (MPa)
  • 700 ° C — R1/1000: 70 N/mm² (MPa); R1/10000: 40 N/mm² (MPa)
  • 800 ° C — R1/1000: 30 N/mm² (MPa); R1/10000: 15 N/mm² (MPa)
  • 900 ° C — R1/1000: 13 N/mm² (MPa); R1/10000: 5 N/mm² (MPa)

O'rtacha sirpanish kuchi (1000 soatdan keyin yorilish, 10 000 soat, 100 000 soat)

  • 600 ° C — Rz/1000: 200 N/mm² (MPa); Rz/10000: 152 N/mm² (MPa); Rz/100000: 114 N/mm² (MPa)
  • 700 ° C — Rz/1000: 90 N/mm² (MPa); Rz/10000: 68 N/mm² (MPa); Rz/100000: 48 N/mm² (MPa)
  • 800 ° C — Rz/1000: 45 N/mm² (MPa); Rz/10000: 30 N/mm² (MPa); Rz/100000: 21 N/mm² (MPa)
  • 900 ° C — Rz/1000: 20 N/mm² (MPa); Rz/10000: 10 N/mm² (MPa); Rz/100000: 8 N/mm² (MPa)

Po'latning mexanik va fizik xususiyatlari

Mexanik xususiyatlar

Maksimal diametri ⌀160 mm bo'lgan novdalar uchun, eritmani yumshatgandan so'ng:

  • Hosildorlik kuchi:
    • Re0,2 (min.): 170 N/mm² (MPa)
    • Re1,0 (min.): 210 N/mm² (MPa)
  • Tortish kuchi Rm: 450–680 N/mm² (MPa)
  • Qattiqlik (maksimal): 192 HB

Fizik xususiyatlar

  • Gęstość: 8,00 g / sm³
  • Chiziqli kengayish koeffitsienti:
    • α20-200 ° C: 15,0 × 10-6 1/K
    • α20-400 ° C: 16,0 × 10-6 1/K
    • α20-600 ° C: 17,0 × 10-6 1/K
    • α20-800 ° C: 17,5 × 10-6 1/K
    • α20-1000 ° C: 17,5 × 10-6 1/K
  • Issiqlik o'tkazuvchanligi:
    • 20°C da: 12 Vt/(m K)
    • 500°C da: 17 Vt/(m K)
  • Maxsus issiqlik: 20°C da 0,55 kJ/(kg K)

Issiqlikka chidamli po'lat 1.4876 / Qotishma 800

1.4876 markali issiqqa chidamli po'lat , X10CrAlNiTi31-20 va uning ekvivalentlari ( 1.4959, Alloy 800, Incoloy 1.4558, Alloy 800H, Alloy 800HP, X5NiCrAlTi31-20, X8NiCrAlTi32-21 ) quyidagi tijorat shakllarida mavjud:

  • Issiqlikka chidamli choyshablar
    • Issiq prokatlangan choyshablar: qalinligi 3 – 50 mm, kengligi 2000 mm gacha, uzunligi 6000 mm gacha
    • Sovuq prokatlangan varaqlar: qalinligi 0,8 – 6 mm, kengligi 1500 mm gacha
    • mijozning chizmasiga muvofiq tayyorlangan shakllar va yonishlar
  • Choksiz quvurlar
    • tashqi diametrlari Ø 10 – 250 mm
    • devor qalinligi 2 – 20 mm
    • tekis qismlar va o'lchamlarga kesilgan qismlar
  • O'ralgan novdalar
    • Dumaloq panjaralar Ø 10 – 250 mm
    • Kvadrat va yassi barlar: 20 × 20 mm dan 200 × 200 mm gacha
  • Soxtalashtirilgan novlar / zarblar
    • vallar, disklar, halqalar va ochiq qolipli zarb qilingan elementlar
    • zarb qilish og'irligi 2000 kg gacha
    • mijozning chizmasiga muvofiq tayyorlangan shakllar

Issiqlikka chidamli po'latlar, issiqqa chidamli zanglamaydigan po'latlar va issiqqa chidamli po'latlar PN 71/H-86022

H5M – ferrit-perlitlitik issiqqa chidamli xrom-molibden po'lati 12CrMo195, 1.7362
H6S2 – ferritli issiqqa chidamli xrom-kremniyli po'lat X10CrAl7, 1.4713
H13JS – ferritli xrom-alyuminiy-kremniyli po'lat X10CrAl13, 1.4724
H18JS – ferritli xrom-alyuminiy-kremniyli po'lat X10CrAl18, 1.4742
H24JS – ferritli xrom-alyuminiy-kremniyli po'lat X10CrAl24, 1.4762
H25T – titan X8CrTi25 qo'shilgan ferritli issiqqa chidamli xrom po'lat, 1.4746
H20N12S2 – ostenitik xrom-nikel-kremniy po'lati X15CrNiSi20-12, 1.4828
H23N13 – ostenitik xrom-nikel po'lati X12CrNi23-13,1.4833
H23N18 – ostenitik issiqqa chidamli xrom-nikel po'lati X12CrNi25-21, 1.4845
H25N20S2 – ostenitik xrom-nikel-kremniy po'lati X15CrNiSi25-20, 1.4841
H16N36S2 – ostenitik nikel-xrom-kremniy po'lati X12NiCrSi35-15, 1.4864

PN ga muvofiq klapan po'lati

H9S2 – perlit-martensit xrom-kremniy klapanli po'lat X45CrSi9-3, 1.4718
H10S2M – perlit-martensit xrom-kremniy klapanli po'lat X40CrSiMo10-2, 1.4731

Issiqlikka chidamli po'lat akk. PN EN 10088-1:2007

1.4876, titan va alyuminiy qo'shilgan X10NiCrAlTi32-21 ostenitik nikel-xrom po'lati 1.4958, qotishma 800
1.4835, X9CrNiSiNCe21-11-2 issiqqa chidamli ostenitik nikel-xrom po'lat, seriy 253 MA® qo'shilgan, Sandvik 253MA®, S30815 

PN EN 10088-1:2007 ga muvofiq turlar ro'yxati

Boshqa yuqori qotishmali va maxsus po'latlar

yuqori haroratlarda ishlash uchun yuqori qotishmali po'latlar
yuqori haroratlarda ishlash uchun qotishma po'latlar
zanglamaydigan po'lat
issiqlikka chidamli va sirpanishga chidamli po'lat
kislotaga chidamli po'latlar

Tez-tez so'raladigan savollar – Issiqlikka chidamli po'lat 1.4876 / Qotishma 800

  1. Issiqlikka chidamli po'lat 1.4876 / Qotishma 800 / Incoloy 800 nima?
    Ushbu yuqori qotishmali ostenitik nikel-xrom po'lati yuqori haroratlarda foydalanish uchun mo'ljallangan. U 1.4876, X10CrAlNiTi31-20, Alloy 800, shuningdek, yuqori samarali versiyalarda Alloy 800H va 800HP sifatida tanilgan.
  2. 1.4876 po'latdan qanday haroratgacha foydalanish mumkin?
    1.4876 po'lati taxminan 1100°C gacha oksidlanishga chidamliligi va strukturaviy barqarorligini saqlab qoladi, bu esa uni juda yuqori haroratlarda ishlaydigan pechlarda, isitish moslamalarida va sanoat uskunalarida ishlatish imkonini beradi.
  3. Qotishma / Incoloy 800 po'lati uchun odatiy qo'llanmalar qanday?
    U ko'pincha quyidagilarda qo'llaniladi:
  • sanoat va metallurgiya pechlarining qismlari,
  • issiqlik almashtirgichlar va isitish tizimlari,
  • kimyo va neft-kimyo uskunalari,
  • quvurlar va yuqori haroratli reaktorlar.
  1. Issiqlikka chidamli 1.4876 po'latni payvandlash mumkinmi?
    Ha, 1.4876 po'lat yaxshi payvandlash qobiliyati bilan ajralib turadi. Biroq, bo'g'inlarning yuqori harorat va sirpanishga chidamliligini ta'minlash uchun plomba metallini to'g'ri tanlash va parametrlarni boshqarish talab etiladi.
  2. Issiqlikka chidamli po'lat 1.4876 uchun qanday yetkazib berish imkoniyatlari mavjud?
    Eng keng tarqalgan takliflar quyidagilarni o'z ichiga oladi:
  • issiq prokatlangan choyshablar, sovuq prokatlangan choyshablar
  • o'ralgan va zarb qilingan panjaralar,
  • choksiz quvurlar,
  • ochiq qolipli zarb buyumlari va maxsus tayyorlangan shakllar.
  1. Alloy / Incoloy 800 va Alloy 800H va 800HP o'rtasidagi farq nima?
    Asosiy marka, Alloy 800 (1.4876), yuqori haroratli xizmat ko'rsatish uchun mo'ljallangan. 800H i 800HP Ular, shuningdek, yaxshilangan sirpanish va uzoq muddatli mustahkamlik parametrlariga ega, shuning uchun ular ekstremal sharoitlarda, ayniqsa uzoq xizmat muddati talab qilinadigan joylarda qo'llaniladi.
  2. Issiqlikka chidamli po'lat 1.4876 ning asosiy afzalliklari nimada?
  • oksidlanish va agressiv gazlarga qarshilik,
  • yuqori haroratlarda strukturaviy barqarorlik,
  • ikki barobar sirpanishga qarshilik,
  • energetika, metallurgiya va kimyo sanoatida keng qo'llaniladi.

Po'lat o'rnini bosuvchi va ekvivalentlari 1.4876, X10NiCrAlTi32-21 (Incoloy 800)

BelgilanishStandart / tizimIshlab chiqaruvchi / mamlakatIzohlar
1.4558EN 10095 / EN 10269EvropaEN (X2NiCrAlTi32-20) ga muvofiq belgi
Qotishma 800Nazwa handlowaMaxsus metallar (AQSh)Asosiy qotishma nomi
Incoloy 800Nazwa handlowaMaxsus metallar (AQSh)Asl savdo belgisi
N08800UNS (ASTM/ASME)AQSHUNS ekvivalenti
NW8800JISYaponiyaYaponcha ekvivalenti
X2NiCrAlTi32-20ENEvropaEN ga muvofiq kimyoviy belgi
Z10NC32-21NFFrantsiyaFransuzcha ekvivalenti
CH20N32TGOST 5632RossiyaRuscha ekvivalenti
CHN32TGOST 5632RossiyaGOSTga muvofiq boshqa belgilar
F-3314 / UNE F-3314UNE 36092IspaniyaIspancha ekvivalenti
FeNi32Cr21AlTiTavsiflovchi belgi-Qotishmaning qisqartirilgan tarkibi
Sanicro 30Nazwa handlowaSandvik (Shvetsiya)Savdo belgisi
Böhler H500Nazwa handlowaBöhler (Avstriya)Tijorat versiyasi Alloy 800
Xeyn 800Nazwa handlowaHaynes (AQSh)Tijorat versiyasi Alloy 800
Coralloy 800Nazwa handlowa-Tijorat ekvivalenti
Unitemp 800Nazwa handlowa-Alloy 800 ning tijorat versiyasi
AL800Nazwa handlowa-Qisqartirish Qotishma 800
Emvac 800Nazwa handlowa-Alloy 800 ning tijorat ekvivalenti
DMV 4958Nazwa handlowaMannesmann (Germaniya)Tijorat versiyasi, issiqlikka chidamli quvurlar
DMV 4959Nazwa handlowaMannesmann (Germaniya)Tijorat versiyasi, issiqlikka chidamli quvurlar
NY800Nazwa handlowaNippon Yakin (Yaponiya)Yaponcha versiyasi Alloy 800
NY811Nazwa handlowaNippon Yakin (Yaponiya)Yaponcha versiyasi Alloy 800
NAS 800Nazwa handlowaNippon Steel (Yaponiya)Alloy 800 ning yaponcha versiyasi
NCF800JIS G4901YaponiyaIncoloy 800 uchun yapon standarti
NCF800HJIS G4901YaponiyaIssiqlikka chidamlilikning ortishi varianti
NCF800HTBJIS G4901YaponiyaYuqori haroratli variant
NCF800HTFJIS G4901YaponiyaYuqori haroratli variant
NCF800HTPJIS G4901YaponiyaYuqori haroratli variant
NCF800TBJIS G4901YaponiyaYuqori haroratli variant
VLX 800Nazwa handlowaVallourec (Fransiya)Alloy 800 ning tijorat versiyasi
Pirad 33Nazwa handlowa-Tijorat versiyasi 1.4558 ga teng
Chronimo 1.4876EN / tijoratGermaniyaAlloy 800H/HT (1.4876) ga o'xshash
Sinoxx 4876Nazwa handlowaGermaniya1.4876 ning tijorat ekvivalenti
EP670Nazwa handlowa-Alloy 800 ning tijorat versiyasi

Cookie sozlamalari

Hurmatli mijozlar, Alfa-Tech veb-sayti to'g'ri ishlashini ta'minlash uchun cookie-fayllardan foydalanadi. Saqlash yoki kirish shartlarini Sozlamalar tugmasini bosish orqali belgilashingiz mumkin. Maxfiylik siyosatimizni o'qib chiqishingizni tavsiya qilamiz.